Visual inspection of the fusion bead is the primary quality check for
HDPE butt fusion joints, defined in DVS 2207-1(
what is DVS2207) for heated-tool welding of HDPE pipes.
- Continuous full-circle double bead
A complete, uninterrupted double bead must run all around the pipe circumference. Broken, partial or discontinuous bead indicates insufficient heating, contamination or unstable welding pressure, which shall be rejected.
- K value requirement (core rule in DVS 2207-1)
The valley between the two bead lobes must stay above the outer pipe surface, which means K>0 at every position around the weld. If the valley sinks below the pipe surface, the joint fails inspection.
- Misalignment limit
Pipe misalignment at the joint shall not exceed 10% of the pipe wall thickness (0.1 × e). Higher offset is not permitted by DVS 2207-1.
- Symmetric bead shape
Both bead lobes on two sides of the weld line should be evenly sized and smoothly rounded. Obvious asymmetry points to poor pipe alignment, tilted heating plate or uneven pressure distribution.
- Surface condition
No cracks, pores, foreign inclusions, sharp notches or cold lines at the bead root. The bead transition from pipe wall to melt rollover shall be smooth.
Important note: Visual check is only preliminary verification. For full quality validation, bend test or destructive test shall be performed as required by the project specification. All welding parameters (temperature, time, pressure) must also comply with DVS 2207-1.
Unqualified HDPE Butt Fusion Beads Qualified HDPE Butt Fusion Beads